1. Chemical composition
Code | KS | JIS | AISI | BS | BS | BS |
Material Grade |
SM30C | S30C | 1030 | 060A30 | 080A30 | 080M30 |
C | 0.27~0.33 | 0.27~0.33 | 0.28~0.34 | 0.28~0.33 | 0.28~0.33 | 0.26~0.34 |
Si | 0.15~0.35 | 0.15~0.35 | agreement | 0.10~0.40 | 0.10~0.40 | - |
Mn | 0.60~0.90 | 0.60~0.90 | 0.60~0.90 | 0.50~0.70 | 0.70~0.90 | 0,60~1.00 |
P | ≦0.030 | ≦0.030 | ≦0.040 | ≦0.050 | ≦0.050 | ≦0.050 |
S | ≦0.035 | ≦0.035 | ≦0.050 | ≦0.050 | ≦0.050 | ≦0.050 |
Ni | <0.20 | <0.20 | - | ≦0.40 | ≦0.40 | ≦0.40 |
Cr | <0.20 | <0.20 | - | ≦0.30 | ≦0.30 | ≦0.30 |
Mo | - | - | - | ≦0.15 | ≦0.15 | ≦0.15 |
Cu | <0.30 | <0.30 | - | - | - | - |
Remark | Ni+Cr<0.35 | Ni+Cr<0.35 | In AISI 3,5,6 C 0.27~0.34 |
- | - | - |
(Referred to KS, JIS, AISI, BS)
2. Mechanical property (SM30C,S30C)
Heat Treatment |
yield point kgf/mm^2 (N/mm^2) |
tensile strength kgf/mm^2 (N/mm^2) |
elongation % |
contraction of area % |
hardness (HB) |
charpy impact value kgf.m/cm^2 (J/cm^2) |
Normalizing 850~900℃ Air cooling |
29≦ (284)≦ |
48≦ (471)≦ |
25≦ | - | 137~197 | - |
Annealing About 840℃ Furnace cooling |
- | - | - | - | 126~156 | - |
Quenching 850~900℃ Water cooling Tempering 550~650℃ Quick cooling |
34≦ (333)≦ |
55≦ (539)≦ |
23≦ | 57≦ | 152~212 | 11≦ (108)≦ |
(Referred to KS, JIS)
'기술' 카테고리의 다른 글
Ultrasonic Testing Code / Standard (초음파탐상시험 규격 / 표준) (0) | 2025.02.04 |
---|---|
Radiographic Testing Code / Standard (방사선투과시험 규격 / 표준) (0) | 2025.02.03 |
SCM430,4130 Material comparison table (0) | 2023.12.31 |
SCM415(KS.JIS) Material comparison table (0) | 2023.12.31 |
SCM435,4135,4137,708A37,34CrMo4 Material comparison table (2) | 2023.12.03 |